1.4310, DIN X12CrNi177, AISI 301
Production specification
Square-shape steel standard Download
Plate steel standard Download
Billet standard Download
Flat bar standard Download
wire standard Download
tube standard Download
pipe standard Download
Forging standard Download
casting standard Download
sheet standard Download
round bar standard Download
coil standard Download
Bar stock standard Download
profiled bar standard Download
1.4310, DIN X12CrNi177, AISI 301
Designation by Standards
Brand Name | Ravne No. | Mat. No. | DIN | EN | AISI |
PK11VZ | 913 | 1.4310 | X12CrNi177 | - | 301 |
Chemical Composition (in weight %)
C | Si | Mn | Cr | Mo | Ni | V | W | Others |
max. 0.12 | max. 1.50 | max. 2.00 | 17.00 | max. 0.80 | 7.50 | - | - | - |
Description
301 is a commonly available austenitic stainless with good corrosion resistance and elevated carbon to allow for cold working to a variety of tempers.
Applications
Automotive trim, kitchen equipment, hose clamps, wheel covers, aircraft components and a wide variety of industrial applications. Springs up to temperature 300oC, pulp cutting machine blades.
Physical properties (avarage values) at ambient temperature
Modulus of elasticity [103 x N/mm2]: 200, 194 (100oC), 186 (200oC)
Density [g/cm3]: 7.9
Thermal conductivity [W/m.K]: 15.0
Electric resistivity [Ohm mm2/m]: 0.73
Specific heat capacity[J/g.K]: 0.50
Coefficient of Linear Thermal Expansion 10-6 oC-1
20-100oC | 20-200oC | 20-300oC |
16.0 | 17.0 | 17.0 |
Hardening
Harden from a temperature of 1010-1120oC followed by water quenching. For thin sections air cooling is acceptable, while heavier sections should be water quenched.
Forging
Hot forming temperature: Commence forging at 1093-1204oC and finish at 927oC.
Machinability
No data.
Corrosion Resistance
This alloy is resistant to the atmosphere, fresh water and mild environments. It will resist oxidation at temperatures up to 840oC.
Welding
All popular techniques may be used, however the material will lose temper in the heat affected weld zone.
Cold working
Most common cold work methods are successful with this alloy. It should be understood however that the material will be more difficult to work than other austenitic stainless steels due its high work hardening rate.
Related hot word search:1.4310 DIN X12CrNi177 AISI 301 1.4310, DIN X12CrNi177, AISI 301 round bar,1.4310, DIN X12CrNi177, AISI 301 forging,1.4310, DIN X12CrNi177, AISI 301 sheet,1.4310, DIN X12CrNi177, AISI 301 coil,1.4310, DIN X12CrNi177, AISI 301 flat bar,1.4310, DIN X12CrNi177, AISI 301 pipe,1.4310, DIN X12CrNi177, AISI 301 Lrregular
Prev:1.4541, DIN X6CrNiTi18-10, AISI 321
Next:1.4401, DIN X5CrNiMo17122, AISI 316
Top
Month Top
- 411.4913*, DIN X19CrMoVNbN11-1
- 351.4138, DIN X120CrMo29-2
- 301.4310, DIN X12CrNi177, AISI 301
- 304140 PH
- 281.3816, DIN X8CrMnN18-18
- 251.4000, DIN X6Cr13, AISI 410S
- 20List of ASTM International standards
- 181.4021, DIN X20Cr13, AISI 420
- 161.4842, DIN X12CrNi2520, AISI 310S
- 151.4305, DIN X8CrNiS18-9, AISI 303